E295GC
(W. NR. 1.0533)
Non-alloy steel for structural purposes
CHEMICAL COMPOSITION: (heat analysis according to the EN 10277-2 standard)
C%
Si %
Mn %
P%
S%
N%
Cu %
FROM
TO
0,045
0,045
0,012
*MECHANICAL FEATURES: (according to the EN 10277-2 standard)
Thickness
mm
Rolled + peeled rolled
(+SH )
hardness HB
510
>1016
>1640
>4063
>63100
140 - 181
140 - 181
140 - 181
Rm (MPa)
470 - 610
470 - 610
470 - 610
Cold drawn
( +C )
Rp0,2 minimum
values
(MPa)
510
420
320
300
255
Rm (MPa)
650 - 950
600 - 900
550 - 850
520 - 770
470 - 740
A5 %
minimum
values
6
7
8
9
9
* Delivery condition: as rolled.
PROPERTIES:
Weldability:
Failing any prescriptions concerning chemical composition, no technical data about this steel
weldability are available.
Notes:
CORRESPONDENCE WITH OTHER STANDARDS ( purely as an indication ) :
EN 10025-2:2004
E295
EN 10025:90
Fe 490-2
UNI 7070
Fe 490
DIN 17 100
St 50-2
NF A35-501
A 50-2