Table 11.
1
Weld defects, description and causes
ISO 6520 Defect Name Description Causes
Defect no.
4011 Lack of side wall fusion Failure of weld metal to fuse to Current too low, travel speed too high,
(Fig. 11.1) weld preparation incorrect torch angle, oxide film on prep.
surfaces, inadequate joint cleaning, weld
preparation too narrow
4012 Lack of inter-run fusion Failure of weld metal to fuse to Current too low, travel speed too high,
(Fig. 11.1) preceding run incorrect torch angle, inadequate
inter-run cleaning
4013 Lack of root fusion Root bead fully penetrated but not Current too low, voltage too low, travel
(Fig. 11.1) fused to root face speed too high, root face too thick, root
gap too wide, incorrect torch angle,
inadequate cleaning
517 Poor restart (cold start) Lack of fusion beneath weld start Incorrect welder technique (see Section
position 7.4.1), poor earthing
402 Lack of penetration Failure to achieve the minimum Current too low, travel speed too high,
penetration specified by design incorrect torch angle, incorrect weld prep.
4021 Insufficient (lack of) root Failure of weld metal to penetrate Current too low, travel speed too fast, root
(Fig. 11.2) penetration fully root faces face too thick, root gap too small,
incorrect torch angle, misalignment
504 Excess penetration Unacceptable protrusion of the root Current too high, travel speed too slow,
(Fig. 11.3) bead root gap too wide, root face too thin
501 Root or face undercut Notch parallel to weld at weld toe. Current too high, travel speed too fast,
(Fig. 11.4) Prevalent at top edge of PB fillet incorrect torch angle, inadequate cleaning
502 (butt) Excess convexity Excess weld metal on the face of a Current too high, travel speed too low,
503 (fillet) Excess weld metal butt or fillet weld incorrect torch manipulation
(Fig. 11.5) (excess cap height)
511 Incomplete fill (face Insufficient weld metal fill giving Poor welder technique, travel speed too
(Fig. 11.6) concavity or missed groove on weld face resulting in fast, current too low, incorrect torch
edge). Insufficient insufficient throat positioning
throat in fillet welds
515 Root concavity Root pass ‘sucked back’ to give a Current too high, root gap too wide, root
(Fig. 11.7) shallow groove face too thin
510 Burn-through Localised loss of weld pool in root Current too high, travel speed too slow,
root face too thin, root gap too large
506 Overlap (roll-over) Weld metal that has rolled over at Weld bead too large, current too high,
(Fig. 11.8) the edges and not fused to the travel speed too slow, prevalent in horiz.–
parent metal. May be face or root vert. welds, inadequate cleaning
201 Porosity Gas entrapped in weld metal giving Dirty consumables, poorly cleaned or dirty
a cavity. May be localised, weld preparations, contaminated shield
uniformly distributed or aligned gas, contaminated (hydrogen containing)
parent metal – especially castings, oxide
film on parent metal, porous gas hoses,
leaks in gas delivery system,
condensation, poor joint design trapping
gas (see Chapter 2)
2016 Worm-hole (piping) Elongated gas cavity formed by Excessive current, travel speed too slow
solidification of large weld pool
2024 Crater pipe Elongated cavity in the weld finish Incorrect welder technique – lack of crater
crater fill
100 Solidification cracking Cracks in weld produced during Incorrect choice of filler metal, failure to
welding control dilution, incorrect edge
preparation, crack susceptible parent
Table 11.1 (cont.)
ISO 6520 Defect Name Description Causes
Defect no.
metal, high restraint, high heat input (see
Chapter 2)
104 Crater cracking Short longitudinal or star-shaped Incorrect welder technique, lack of crater
crack in finish crater fill
100 Liquation cracking Cracking in the HAZ or in Incorrect filler metal, crack sensitive
previously deposited weld metal parent metal, high restraint, high heat
input (see Chapter 2)
303 Oxide entrapment Oxide films trapped within the Oxide films in or on parent metal, oxide
weld metal films in or on filler metal, oxygen in shield
gas, poor gas shielding, inadequate
cathodic cleaning
3034 Puckering Excessive oxide entrapment from Poor gas cover, very high weld current
weld pool turbulence
3041 (tungsten) Tungsten or copper Accidental contact of the electrode Poor welder technique, incorrect
3042 (copper) inclusions (TIG) or contact tip (MIG) mechanised set-up
602 Stray arc strike Accidental arcing outside weld prep. Welder carelessness
602 Spatter Droplets of weld metal expelled Poor welder technique, incorrect weld
from weld pool parameters
606 Under ushing Thinning below design thickness Excessive grinding
Weld defects and quality control 203
Lack of Inter-run Fusion
Lack of Root Fusion
Lack of Side Fusion
11.1
Defects 4011 lack of side wall fusion, 4012 lack of inter-run
fusion, 4013 root fusion.
Insufficient penetration
11.2
Defect 4021.
EP
Excessive penetration (EP)
11.3
Defect 504.
UC
UC
Excessive undercut
11.4
Defect 501.
(a) Butt
EC
(b) Fillet
Excessive convexity
11.5
(a) Defect 502. (b) Defect 503.
IF
Incomplete filling or underfill
Insufficient ‘throat’
11.6
Defect 511.
RC
Root concavity (RC)
11.7
Defect 515.
Overlap
11.8
Defect 506.
Weld defects and quality control 205
static or dynamic loading, temperature and corrosive conditions and the
consequences of failure.
11.3 Non-destructive testing methods
NDE may be used to reveal defects that would be difficult or impossible to
detect by visual examination. The techniques are used during manufacture
as a quality control tool to determine the quality of the work. The extent
of NDE depends upon the application and the criticality of the joint and is
generally specified in the relevant application standards or contract speci-
fication. It is important for NDE to be included in the planning of the
fabrication process as it can require substantial time and resources. Full
account of this must be taken if disruption of production and delays to the
programme are to be avoided.
The requirement to perform NDE must also be taken into account during
the design phase. As with welding, access for NDE must be planned into
the component. The implication of this is that both welding engineers and
designers must be conversant with the techniques and their limitations if
the processes are to be used effectively.
11.3.1 Penetrant examination
This is a technique that is capable of detecting surface breaking defects only.
It relies upon a coloured or uorescent dye, sprayed upon the surface,
penetrating these defects. After cleaning the excess from the surface, the
dye within the defect is drawn to the surface by spraying on a developer in
the case of the colour contrast dye or by exposing the surface to ultra-violet
light. The defect is revealed by the dye staining the developer or by
uorescing (Fig. 11.9).
Figure 11.10 is a photograph of a typical penetrant examination indica-
tion. The uorescent dye gives greater sensitivity than the colour contrast
dye and does not require the use of a colour contrast developer but does
require the use of an ultra-violet light and preferably a darkened [Link]
cleaners, penetrant dyes and developers can all be obtained in aerosol cans,
making the process extremely portable and ideal for site use.
The dye used as a penetrant must be capable of penetrating narrow
cracks but must not be removed from more open defects during the clean-
ing operation carried out before the application of the developer. The dye
must have a high contrast with the developer. It is important that the test
piece is thoroughly pre-cleaned – any dirt, oil or water in the crack may
prevent the penetrant from entering. Degreasing should be carried out by
swabbing or immersing the item in one of the proprietary cleaners, acetone
or methanol. Immersion in an ultrasonic cleaning bath is probably the best
206 The welding of aluminium and its alloys
Defect open to surface Penetrant
Penetrant drawn into
defect
Penetrant drawn out
Penetrant cleaned off
and staining developer
but retained in defect
Developer sprayed on
Beam of fluorescent light
Dye fluorescing
Fluorescent dye retained
in defect
11.9
Penetrant examination principles.
11.10
Liquid penetrant test result illustrating staining of the spray-on
developer by a defect in the HAZ. Courtesy of TWI Ltd.
method. Wire brushing or grinding should not be used unless it can be fol-
lowed by an acid etch as mechanical methods of cleaning can smear over
defects and prevent the dye from penetrating.
Inspection in other than the at position is difficult but penetrants have
been developed with a jelly-like consistency that can be used to carry out
inspections in the vertical and overhead positions. Automated methods may
be used, with the components loaded into baskets and processed on a con-
206 The welding of aluminium and its alloys
Defect open to surface Penetrant
Penetrant drawn into
defect
Penetrant drawn out
Penetrant cleaned off
and staining developer
but retained in defect
Developer sprayed on
Beam of fluorescent light
Dye fluorescing
Fluorescent dye retained
in defect
11.9
Penetrant examination principles.
11.10
Liquid penetrant test result illustrating staining of the spray-on
developer by a defect in the HAZ. Courtesy of TWI Ltd.
method. Wire brushing or grinding should not be used unless it can be fol-
lowed by an acid etch as mechanical methods of cleaning can smear over
defects and prevent the dye from penetrating.
Inspection in other than the at position is difficult but penetrants have
been developed with a jelly-like consistency that can be used to carry out
inspections in the vertical and overhead positions. Automated methods may
be used, with the components loaded into baskets and processed on a con-
208 The welding of aluminium and its alloys
be placed either side of a thin plate-like sample or can be wound to give
side-by-side coils in a single probe. These may be shaped to fit in the bore
or around the outside of pipes and tubes and in these applications the process
lends itself to automation. The equipment is calibrated using a defect-free
specimen. The accuracy can be affected by metallurgical condition, stand-
off and coil dimensions. For these reasons eddy current testing is used only
rarely on welded components, although it is excellent in examining contin-
uously welded tube from pipe mills. The process has been developed over
recent years to make it more portable and simpler to use. Microprocessor-
based control and recording units, improved and more tolerant probes and
light-weight electronics have enabled the technique to be used on-site for
the examination of structures in service, where it is an effective tool for the
detection of cracking and corrosion problems. It is also possible for the
depth of surface cracks to be determined. It is of limited use for interro-
gating welds, however, being most commonly used in the examination of
continuously welded tube, and is not covered further in this chapter.
11.3.3 Ultrasonic examination
The ultrasonic examination of welds uses the same principles as when sonar
is used for the detection of submarines. A ‘sound’ wave emitted from a
transmitter is bounced off an object and this re ection captured by a
receiver. The direction and distance of the object can be determined by
measuring the elapsed time between transmission and detection of the
‘echo’. In welded components this is usually done by moving a small probe,
containing both transmitter and receiver, over the item to be examined and
displaying the echo on an oscilloscope screen. The probe transmits a beam
of ultrasound that passes through the metal and is re ected back from any
defects, much like shining a torch at a mirror, in principle with the same
rules applying to the re ection of the beam. This is illustrated in Fig. 11.11.
Deeply buried defects such as lack of fusion, lack of penetration and cracks
in addition to volumetric defects such as slag entrapment and porosity are
all easily detected.
The success of the technique depends upon the use of trained, experi-
enced operators who know precisely the characteristics of the metal being
examined, the beam direction, its amplitude and frequency and the weld
geometry. It is recommended that operators should be approved to one of
the certification schemes such as those operated by the BINDT or the
ASNT.
The frequency of the ultrasonic waves is generally in the range of 2–
5 MHz, the lower frequencies being used for the examination of coarse-
grained material and on rough surfaces. The higher-frequency probes are
used for the detection of fine defects such as cracks, non-metallic inclusions,
11.3.4 Radiographic examination
Electromagnetic radiation has properties that are useful for industrial radi-
ography purposes. The rays travel in straight lines and cannot be de ected
or re ected by mirrors or lenses; they have wavelengths that enable the
radiation to penetrate many materials, including most metals. They will,
however, damage living tissue and therefore present some health and safety
problems.
The radiation, either X-rays from a suitable source or gamma rays from
a radioactive isotope, is absorbed as it passes through the material. This
absorption increases as the density of the material increases so that if a pho-
tographic film is placed on the side opposite the radiation source, any less
dense areas will appear as darker areas on the film (Figs. 11.14 and 11.15),
to give a shadow picture of the internal features of the test sample once the
film has been processed. Thus voids, porosity, slag, cracks and defects of
212 The welding of aluminium and its alloys
Source of radiation
Cavity
Image of
Weld
cavity on film
Film
Intensifying screens
Anti-back-scatter backing
11.14
Principles of radiographic examination of a weld. Courtesy of
TWI Ltd.
(a)
(b)
11.15
Radiograph of aluminium welds.
(a) Longitudinal cracking at the weld start. Close square TIG butt weld
in 7000 series alloy. (b) Gross porosity in TIG butt weld in 4000 series
alloy.
Weld defects and quality control 213
geometry can all be identified, although planar defects normal to the beam
may not be detected.
To radiograph a welded joint a suitable source of radiation, a film in a
light-proof cassette and some method of processing the film are required.
This latter generally requires a dark room where the film can be developed,
fixed, washed, dried and viewed. The radiation can be produced from an X-
ray tube, the energy generally being described by the voltage and current
at which the tube is operated. These may vary from 20 kV to 30 MV and 10
to 30 mA, although the normal limit for the commonly available industrial
units is around 400 kV. A 400 kV unit is capable of penetrating up to
100 mm of steel and 200 mm of aluminium. Gamma radiation is produced
by the decay of a naturally occurring or manufactured radioactive isotope.
The isotopes decay over a period of time, a measure of the longevity of the
source being the
half life
, the length of time taken for the source to decay
to half of its initial intensity. The most common isotopes are cobalt-60, half
life 5.3 years; caesium-137, half life 30 years; iridium-192, half life 74 days;
thulium-170, half life 127 days and ytterbium-169, half life 31 days. The
strength of the source is expressed as curies or becquerels. As a gamma ray
source cannot be switched off the isotope is stored in a special container
equipped with either a port that can be opened remotely to expose the
source or from which it can be wound out when required (Fig. 11.16).
(a)
Collimating
head
Teleflex
Source
cable
Shielding
Winding
mechanism
(b)
11.16
Radioactive isotope projection system. Courtesy of TWI Ltd.