The document outlines the Post Weld Heat Treatment (PWHT) cycle times for various ASME materials as per ASME Section VIII, Division 1. It provides specific temperature, heating rates, soaking times, cooling rates, and thickness limits for different grades of materials. The table serves as a reference for ensuring compliance with PWHT requirements in welding processes.

Uploaded by

Hary adi
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
153 views1 page

PWHT Table For ASME Material-Sec VIII

The document outlines the Post Weld Heat Treatment (PWHT) cycle times for various ASME materials as per ASME Section VIII, Division 1. It provides specific temperature, heating rates, soaking times, cooling rates, and thickness limits for different grades of materials. The table serves as a reference for ensuring compliance with PWHT requirements in welding processes.

Uploaded by

Hary adi
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 1

PWHT CYCLE TIME AS PER ASME CODES FOR ASME MATERIALS

P # & Material PWHT


ASME Sec VIII , Div 1
Sr # P# Gr # Grade Temperature Min Ref: Table UCS - Heating rate Thickness Limits Ref: Table UCS - Governing Thickness for
Soaking time Ref: Table UCS -56 Cooling rate Ref: UCS -56 (d) (5) Preheat Temperature
56 Ref : UCS -56 (d) (2) 56 PWHT(Socket Welding)

1 SA 36 ,SA 53 ,SA 106 Gr B

2 SA234 WPB, SA 283 GR A


1 1) 595˚C (1100˚F) Above 425˚C , the rate shall not Above 425˚C , the rate shall not 1) For Nominal Thickness above
3 SA 333 Gr 6, sa 350 Gr Lf1 1) Up to 2" Thickness, 1Hr /Inch (
-For Gr 1,2 & 3. more than 222˚C / Hr divided by more than 280˚C / Hr divided by 1.5" ( 38.0 mm) & For Thickness Sahll not be less than 0˚C.If
25.0 mm), But Min 15 Minutes.
maximum Thickness of Shell or maximum Thickness of Shell or from 1.25" (32.0 mm) to 1.5" surface temperature goes below
4 1 SA420 WPL6, SA 516 GR 60 2) For 2" to 5" Thickness 2 Hr Plus
Header (in Inches), But Any case Header (in Inches) & Not Less (38.0MM) if Preheat is 0˚C , then to be preheated to
15 Minnutes for each additional
5 SA 105, SA 216 WCB,SA 234 WPC not exceed 222˚C / Hr & Not Less than 56˚C /Hr. From 425˚C , Cool maintained at 95˚C during Minimum of 15˚C ( UW -30)
of 25.00 MM over 2" Thickness.
than 56˚C /Hr. in Still Air. Welding.Note C of table UCS-56
6 2 A 350 GR LF2,SA 516 GR 70
2) For Gr # 4 Not Applicable
7 SA 671 GR CC 70 CD 70

8 A 204 GR A, SA209 GR T1B


1) For Gr # 3 , Not Mandatory
1) Up to 2" Thickness, 1Hr /Inch (
9 1 SA 213 T2,SA 234 WP1, SA 335 P1
25.0 mm), But Min 15 Minutes. Above 425˚C , the rate shall not more Above 425˚C , the rate shall not more Sahll not be less than 0˚C.If
than 222˚C / Hr divided by maximum than 280˚C / Hr divided by maximum 2) For Gr # 1 ,2 Thickness ≤ 16 mm,
10 SA 356 GR 2, SA 691 CM-65 595˚C ( 1100˚F) -For Gr 1,2 & surface temperature goes below
3 Thickness of Shell or Header (in Thickness of Shell or Header (in unless PQR Thickness ≥ Production
3. Inches), But Any case not exceed Inches) & Not Less than 56˚C /Hr. Weld Nominal Thickness, Not 0˚C , then to be preheated to
11 A 182 GR F2, GR F1 , SA 204 GR C required. Minimum of 15˚C ( UW -30)
222˚C / HR & Not Less than 56˚C /Hr. From 425˚C , Cool in Still Air.
2
12 SA 336 GR F1 3) For Other Conditions , Refer Code.

13 A 182 FL12, CL.1,2


1) Up to 2" Thickness, 1Hr /Inch ( 25.0
14 A 213 T11 / T 12 mm), But Min 15 Minutes.
1) Not Mandatory for D ≤ 100.0 MM ,
1 T ≤ 16.0 MM , Max C = 0.15% &
15 A 234 WP11 / 12 Cl.1,SA 335 P11 Above 425˚C , the rate shall not more Above 425˚C , the rate shall not more Preheat maintained at 120˚C
Sahll not be less than 0˚C.If
than 222˚C / Hr divided by maximum than 280˚C / Hr divided by maximum
2) Over 2"(50mm) to 5" ( 125mm) = 1Hr surface temperature goes below
16 4 A 335 P12 ,SA 336 GR F12/F11 650˚C ( 1200˚F) -For Gr 1,2 /Inch
Thickness of Shell or Header (in Thickness of Shell or Header (in
Inches), But Any case not exceed Inches) & Not Less than 56˚C /Hr.
0˚C , then to be preheated to
17 2 A 333 GR 4 222˚C / HR & Not Less than 56˚C /Hr. From 425˚C , Cool in Still Air. Minimum of 15˚C ( UW -30)
2) Others Refer UCS -56 of Sec VIII ,
18 A 148 90 -60 Div -1
3
19 A 668 Cl.kb, ka, kc

20 SA 182 F22, Cl.1 , Cl.3, F21

21 SA 213 T21 & T 22, SA 217 GR WC9

22 SA 234 WP22, Cl.1,


1) Up to 2" Thickness, 1Hr
23 5A 1 A 335 GR P21 & 22 /Inch ( 25.0 mm), But Min 15
Minutes.
24 A 336 F22 Cl.1 & Cl.3, SA 336 F21 CL.1

25 SA 369 FP21 & 22, SA 369 FP21 & 22


675˚C ( 1250˚F)
26 A 691 2.25 CR, Cl.1 & 2
Above 425˚C , the rate shall
27 A 182 F5a , F5 & F9, SA 234 EP5 & WP9 Above 425˚C , the rate shall
not more than 222˚C / Hr
not more than 280˚C / Hr Sahll not be less than 0˚C.If
28 A 213 T5c, T5, T5b &T 9 divided by maximum Thickness Refer UCS -56 Page # 164 of
divided by maximum Thickness surface temperature goes below
of Shell or Header (in Inches), ASME Sec VIII, Div -1 - 2007 ,
of Shell or Header (in Inches) 0˚C , then to be preheated to
29 1 A 335 GR P5, 5b & 5c , P9 But Any case not exceed 222˚C 209b Addenda.
& Not Less than 56˚C /Hr. Minimum of 15˚C ( UW -30)
/ HR & Not Less than 56˚C
30 A 336 F5, F5a & F9 ,369 GR FP5 &FP9 2) Over 2"(50mm) to 5" ( From 425˚C , Cool in Still Air.
5B /Hr.
31 SA 387 5 Cl.1 & 2 , SA 691 5 CR, Cl.1 & 2 125mm) = 1Hr /Inch

32 A 213 T91

33 2 A 217 GR C12A Not Given

34 A 356 GR 12A

35 A 182 F 3V, F3 VCb,F22V


3) Over 5" Thickness , 5hrs +15
35 5C 1 A 336 F3VCb , F3V & F22V 650˚C ( 1200˚F) -For Gr 1,2 Minutes for Each Additional inch Over
2"(50 mm).
37 A 508 22 Cl.3 & 3V ,SA 542 22 Cl3 & 3V

38 SA-182 F6a Cl 1,2,3 & 4, F6b

39 6 1,2 & 3 SA217 CA15,SA240 Type 410, 429 Not Given in Code NA NA NA NA NA NA

40 SA268 Type 410, SA 336 F6,SA 351 CA15

41 SA182 F430,SA 240 Type 405,409,410S


7 1&2 Not Given in Code NA NA NA NA NA NA
42 SA240 S44400,SA268 Type 439

43 A 182 FR , SA 203 Gr A,B, SA 234 WPR


Sahll not be less than 0˚C.If
44 A 333 GR 7 & GR 9, SA 334 GR 7 & 9 Refer UCS -56 Page # 166 of
1hr Minimum, Plus 15 Minutes surface temperature goes below
9A 1 595˚C ( 1100˚F) Above 425˚C , the rate shall not Above 425˚C , the rate shall not ASME Sec VIII, Div -1 - 2007 ,
/Inch Over 1"(25.0 mm) 0˚C , then to be preheated to
45 A 350 GR LF5, Cl 1&.2 , SA 350 GR LF9 more than 222˚C / Hr divided by more than 280˚C / Hr divided by 209b Addenda. Minimum of 15˚C ( UW -30)
maximum Thickness of Shell or maximum Thickness of Shell or
46 SA 714 Gr v, Tp.E , Gr V
Header (in Inches), But Any case Header (in Inches) & Not Less
47 A 203 Gr D , Gr. E & F not exceed 222˚C / HR & Not Less than 56˚C /Hr. From 425˚C , Cool
Sahll not be less than 0˚C.If
than 56˚C /Hr. in Still Air. Refer UCS -56 Page # 167 of
1hr Minimum, Plus 15 Minutes surface temperature goes below
48 9B 1 A 333 GR 3 , SA 334 GR 3 595˚C ( 1100˚F) ASME Sec VIII, Div -1 - 2007 ,
/Inch Over 1"(25.0 mm) 0˚C , then to be preheated to
209b Addenda.
49 A 350GR LF3 , SA 765 III Minimum of 15˚C ( UW -30)

50 SA 479 S32550
10 1 Not Given NA NA NA NA NA NA
51 SA 815 S 32760

52 Alloy S31803

53 10H 1 Alloy S32550 Not Given NA NA NA NA NA NA

54 Alloy S32750

55 SA 240 XM-33,27,SA268 TP446


10 I 1 Not Given NA NA NA NA NA NA
56 SA479 XM-27,SA 268 & 731 XM-27,33

57 SA 182 F91,A217 CA12A,SA234WP91 1) Up to 5" Thickness, 1 Hr/Inch (


2.0 Min / MM) , 30 Mints Sahll not be less than 0˚C.If
minimum . surface temperature goes below
58 15 E 1 SA336 F91,SA369F91,A356 12A 720°C Same as P # 9A Same as P # 9A ALL Thickness
2) For above 5" Thickness, 5hr 0˚C , then to be preheated to
Plus 15 Mints for each additional Minimum of 15˚C ( UW -30)
59 A691 91,EN10222-2 X10CrMoVNb9-1 Inch.

Note

1 The above table is prepared based on ASME Code edition 2010 addenda 2011a