GB/T 9756-2018 (English Version) Synthetic resin emulsion coatings for interior wall
GB/T 9756-2018 (English Version) Synthetic resin emulsion coatings for interior wall
ICS 87.040
G 51
(English translation)
https://www.chinastandard.net/i/GBT9756-2018.html
https://www.ChinaStandard.net -> Buy the full version PDF
Contents
Foreword ........................................................................................................................... II
1 Scope .......................................................................................................................... 1
2 Normative references .................................................................................................. 1
3 Product classification and grading ............................................................................... 2
4 Requirements .............................................................................................................. 2
5 Test methods ............................................................................................................... 2
6 Inspection rules ........................................................................................................... 8
7 Marking, packaging and storage.................................................................................. 8
Annex A (Normative) Alkali burnout resistance test methods ......................................... 9
https://www.chinastandard.net/i/GBT9756-2018.html
https://www.ChinaStandard.net -> Buy the full version PDF
1 Scope
This standard specifies the product classification and grading, requirements, test methods,
inspection rules as well as marking, packaging and storage of the synthetic resin emulsion
coatings for interior wall.
This standard is applicable to the coatings for interior wall, which are made from a mixture
of pigments, extender pigment and various additives with the synthetic emulsion as base
material and formed into a thin coating layer with smooth surface after application,
including primer and finishing coat.
2 Normative references
The following referenced documents are indispensable for the application of this
document. For dated references, only the edition cited applies. For undated references,
the latest edition of the referenced document (including any amendments) applies.
GB/T 1728-1979 Methods of test for drying time of coatings of paints and putties
GB/T 1766-2008 Paints and varnishes - Rating schemes of degradation of coats
GB/T 1910 Newsprint
GB/T 3186 Paints, varnishes and raw materials for paints and varnishes -
Sampling
GB/T 6682-2008 Water for analytical laboratory use - Specification and test methods
GB/T 6750-2007 Paints and varnishes - Determination of density - Pyknometer
method
GB/T 8170-2008 Rules of rounding off for numerical values & expression and
judgment of limiting values
GB/T 9265-2009 Determination for alkali resistance of film of architectural paints and
coatings
GB/T 9266-2009 Determination of scrub resistance of film of architectural paints and
coatings
GB/T 9268-2008 Determination of freeze-thaw resistance of latex and emulsion paints
GB/T 9271-2008 Paints and varnishes - standard panels for testing
GB/T 9278 Temperatures and humidities for conditioning and testing of paint
specimens.
GB/T 9750 Marks for package of coating products
GB/T 13491-1992 General rule for packing of coatings
GB/T 15608 The Chinese color system
GB/T 23981-2009 Determination of contrast ratio of white and light coloured paints
https://www.chinastandard.net/i/GBT9756-2018.html
https://www.ChinaStandard.net -> Buy the full version PDF
A.3.1 Add test solution (A.1.2) into the test container (A.1.4) to such a level that is
slightly higher than the height of the underlaid porous barrier.
A.3.2 Carefully put the test plate (A.2) into the container, with the primer surface brushed
with iron blue upward; the test plate shall be immersed in the test solution to a depth
greater than two thirds of the test plate thickness to ensure that all the bottom surfaces of
the test plate are fully moistened by the test solution within the test cycle. Cover the
chamber mouth with newsprint with a density of ≥0.045 kg/m2 and ≤0.051 kg/m2 in
accordance with the requirements of GB/T 1910 and seal the perimeter edges with
adhesive tape well.
A.3.3 Prepare 5 pieces for each sample parallelly and carry out the test according to the
test time specified in Table 1; at the end of the test, take out the test plate, which shall be
kept upright to ensure that the test plate is ventilated and all dried, place it for 24h under
the test environment specified in 5.2 and observe the result.
A.3.4 During the test cycle, attention shall be paid not to touch the test chamber (it may
be placed at an unaccessible position); once the test plate is submerged in the solution,
this test shall be deemed as invalid. Where the test plate is placed in the solution,
attention shall be paid that the solution shall not contaminate the test plate surface and
any small-area contamination shall be marked by drawing a circle with a marking pen and
this position is not observed after completion of the test. The covering newspaper shall not
be lifted up within the test cycle. Where the test plate is taken out after completion of the
test, attention shall be paid that the solution shall not contaminate the test plate surface
and any small-area contamination shall be timely marked by drawing a circle with a
marking pen and this position is not observed after the test plate is dry.
During the judgment, observe the middle area of the test plate, with the observation area
of (110×50)mm2 (subject to the area calculated by multiplying the long side length minus
40mm by the short side length minus 20mm of the test plate), observe the percentage of
iron blue discoloration (from blue to brown yellow) area; if respective discoloration area of
at least three among the five test plates is not greater than 10%, it will be judged as
"normal".
11
https://www.chinastandard.net/i/GBT9756-2018.html